Skip to main content Skip to footer

Corrosion Assessment of an Aluminum-Framed Curtain Wall

May 15, 2007

CORROSION ASSESSMENT OF AN
ALUMINUMFRAMED
CURTAIN WALL
BY FUSHUANG CUI AND MARK SCHMIDT
WISS, JANNEY, ELSTNER ASSOCIATES, INC., NORTHBROOK, IL
S Y M P O S I U M O N B U I L D I N G E N V E L O P E T E C H N O L O G Y • NO V E M B E R 2 0 0 7 C U I A N D S C H M I D T • 2 1
ABSTRACT
The corrosion condition of an aluminumframed
curtain wall of a 14story
office building
was evaluated. The investigation included onsite
inspection and testing, as well as laboratory
analyses. Techniques employed included screw pullout
tests, chloride analyses,
Scanning Electron Microscopy/Energy Dispersive Xray
Spectroscopy (SEM/EDS) and
Fourier Transformed Infrared Spectroscopy (FTIR). The vertical mullions were all painted
and little corrosion was observed. For the horizontal mullions, corrosion was concentrated
at occluded areas; namely, the connections where the stainless steel screws were in contact
with aluminum pressure plates and screw chases. A significant amount of chloride (approximately
1 percent by weight) was detected in the corrosion products and SEM/EDS confirmed
the presence of the chlorine element. The chloride was likely from airborne deicing
salts. It was speculated that the widespread water leakage, inherent crevices, dissimilar
metals, and presence of chloride were responsible for the observed corrosion. The degree of
corrosion was found to correlate very well with screw pullout
strength: more advanced corrosion
corresponded to lower pullout
strength values. Despite the corrosion, all the tested
screw connections had high remaining strength and it was projected that the screw connections
would retain sufficient strength to resist current coderequired
wind loads for at
least another 20 years of service.
SPEAKER
MARK SCHMIDT — WISS, JANNEY, ELSTNER ASSOCIATES, INC., NORTHBROOK, IL
During his 22 years experience at Wiss, Janney, Elstner Associates, Inc., MARK
SCHMIDT has focused on the assessment, preservation, remedial design, contract document
preparation, and implementation of restoration programs for a variety of building
envelopes. He has led investigations involving glass and aluminum curtain walls, precast
concrete panels, thin stone veneers, stone and brick masonry, terra cotta, sliding door and
window assemblies, composite panels, exterior insulation and finish systems (EIFS),
mosaic tile systems, and stucco systems.
These investigations have addressed water infiltration conditions, including systematic
sealant failures; surfacerelated
distress, such as cracked and spalled concrete or masonry
stained or etched glass, corroded aluminum or steel components, and paint or coating failures;
glass breakage, failure of insulating glass units, and composite panel distress; and
structural failure involving mechanical anchorage and structural silicone glazing.
Mr. Schmidt is a member of the ASCE and the ASTM. He has authored papers and presented
seminars and short courses on potential problems and preventive maintenance of
curtain walls. He has also coauthored a chapter in a book titled Structural Condition
Assessment.
2 2 • C U I A N D S C H M I D T S Y M P O S I U M O N B U I L D I N G E N V E L O P E T E C H N O L O G Y • NO V E M B E R 2 0 0 7
CORROSION ASSESSMENT OF AN
ALUMINUMFRAMED
CURTAIN WALL
Figure 1 – An overview of the 14story
building.
INTRODUCTION
The curtain wall of a 14story
office building (Figure 1)
in the Chicago suburbs was
manufactured and installed in
approximately 1980. It consists
primarily of alternating
horizontal bands of vision and
spandrel glasses that comprise
approximately 4,400 distinct
glazed openings. Each glass
product is supported on four
sides by aluminum framing
and exteriormounted
pressure
plates. Rubber setting
blocks and gaskets separate
the glass from the aluminum
framing and pressure plates.
A crosssection
of the typical
pressure plate configuration
taken from the curtain
wall shop drawings is given in
Figure 2. The exterior pressure
plates resist wind loads that
create suction on the glass.
Stainless steel screws are used
to fasten the pressure plates to
serrated screw chases in both
the horizontal and the vertical mullions.
Most of the exterior pressure plates are concealed
with cosmetic aluminum snapon
covers. Figure 3 shows a horizontal pressure
plate and a snapon
cover, both containing a
series of weep holes that
allow water, which has
penetrated into the glazing
pocket, to drain back
to the exterior.
The authors’ firm was
retained by the building
owners to develop plans
and specifications for
sealant repairs to address
widespread water leakage
problems in the curtain
wall. During a related site
visit, two horizontal pressure
plates and one vertical
pressure plate were
removed from the west
elevation. In the screw
chase of one horizontal mullion at the sill of had been engaged. In addition, a thin foam
a floor spandrel opening, a white powdery tape was present at the interface between
substance (see Figure 4) was observed at the pressure plate and the mullion (see
locations where the stainless steel screws Figure 5). No significant amount of white
Figure 2 – Cross section of typical pressure plate configuration (reproduced from the curtain wall
shop drawings).
S Y M P O S I U M O N B U I L D I N G E N V E L O P E T E C H N O L O G Y • NO V E M B E R 2 0 0 7 C U I A N D S C H M I D T • 2 3
substance was observed at the screw chase
of the other horizontal mullion, which was
located at the sill of a vision opening where
no foam tape was present. The adjacent vertical
mullion also had no signs of the white
substance within its screw chase.
Preliminary analyses by Scanning
Electron Microscopy/Energy Dispersive Xray
Spectroscopy (SEM/EDS) of the sampled
white substance and the foam tape
suggested that the substance was aluminum
corrosion product with some chlorine
and calcium content. The foam tape
was also found to contain chlorine and calcium.
It was therefore suspected that the
observed aluminum corrosion was the
result of an otherwise benign galvanic corrosion
cell between the stainless steel screw
and the aluminum
mullion
that had been
energized by the
Figure 3 – Horizontal presence of free
pressure plate (top) and chloride. This
interior of snapon
phenomenon was
cover (bottom). unusual in that
deleterious galvanic
corrosion
between alumiFigure
4 – Initial severe num and stainless
steel is
rarely, if ever,
reported in curtainwall
construction.
Due to the
corrosion site.
Figure 5 – Foam tape at
pressure plate/mullion uncertainty of the
interface. longterm
effect
of the corrosion
on the structural
integrity of the
pressure plate
connections, further investigation was warranted.
The building owners retained the authors’
firm to perform further investigation of this
condition to determine the extent, cause, and
ramifications of the aluminum corrosion and to
determine the scope of corrosionrelated
repairs, should they be deemed necessary. The
investigation included onsite
observation,
sampling, and testing, as well as laboratory
analyses.
METHODOLOGY
ONSITE
OBSERVATIONS AND SAMPLING
In an attempt to determine the extent and
possible pattern of the ongoing aluminum corrosion,
the following activities were performed
at 41 façade inspection openings distributed on
2 4 • C U I A N D S C H M I D T S Y M P O S I U M O N B U I L D I N G E N V E L O P E T E C H N O L O G Y • NO V E M B E R 2 0 0 7
Location Type Inspected
openings
Total openings
on building
Percent
inspected
Regular VOs 1 16 1560 1.0
Corner VOs 2 2 288 0.7
Regular SOs 3 14 1690 0.8
Corner SOs 4 2 312 0.6
Ground level VOs 5 4 296 1.4
Ground level SOs 6 3 296 1.0
VO – vision opening; SO – spandrel opening
Table 1 – Opening type and percent inspected.
11 swing stage drops and at various floors
of the building:
• Documentation and rating of the
corrosion condition of the screw
sites on the pressure plates and
screw chases using a relative rating
system developed for this project
• Visual comparison of cleaned, corroded
aluminum surfaces at screw
engagement with adjacent corrosionfree
aluminum surfaces
• Sampling of powdery materials and
foam tapes for
laboratory analyses
TESTING
To identify possible
cause of corrosion and
assess corrosioninduced
system capacity
loss, the following tests
were performed:
• Onsite
testing
— Chloride conc
e n t r a t i o n
tests on exterior
surfaces
of selected
p r e s s u r e
plates using
commercial
chloride testing
kits
— Mechanical
pullout
tests
on selected
s t a i n l e s s
steel screws
engaged in
a l umi n um
screw chases
using custom
test apparatus
• Laboratory testing of powder samples
— SEM/EDS
— Fourier Transformed Infrared
Spectroscopy (FTIR)
— XRay
Diffraction (XRD)
— Chloride analyses
• Laboratory testing of foam tapes
— SEM/EDS
— FTIR
The three laboratory test techniques
(SEM/EDS, FTIR, and XRD) are complimentary
to one another and allow possible
characterization (i.e., identification of elements
and chemicals) of the powdery materials
and foam tapes.
FINDINGS
ONSITE
OBSERVATION AND SAMPLING
The curtain wall openings were divided
into six different types based on their locations.
Table 1 lists the classification of the
openings and the percentage of opening
types inspected.
The vertical mullions were all painted
and exhibited insignificant levels of corrosion
(see Figure 6). The investigation
focused, therefore, on the unpainted horizontal
members.
The screw chases of the horizontal mullions,
which have a mill finish, were corroded
to varying degrees. Corrosion ratings
developed for individual screw sites within
the screw chases (listed in increasing magnitude
of corrosion activity) included trace,
moderate, heavy, and severe (see Figure 7).
While a few sporadic screw sites (approximately
2 percent of the total sites observed)
were rated as severe, the vast majority
was rated as trace or moderate,
and the average rating was between
Figure 6 – Vertical members
exhibited trace, if any, corrosion
activity: (a) condition of a pressure
plate (left); (b) condition of a
painted screw chase (above).
S Y M P O S I U M O N B U I L D I N G E N V E L O P E T E C H N O L O G Y • NO V E M B E R 2 0 0 7 C U I A N D S C H M I D T • 2 5
trace and moderate.
Figure 8 shows the condition of a screw
Figure 7 –
Varying
corrosion
conditions:
A) trace; B)
moderate;
C) heavy; D)
severe.
A
B
C
D
site rated as “severe” before and after cleaning
was performed. The extent of aluminum access difficulty. sion activity also varied significantly. A simsection
loss in the screw chase was difficult The exterior surface of the horizontal ilar corrosion rating system (Figure 9) was
to measure or otherwise quantify due to pressure plates often exhibited corrosion used to assess the condition of these comlocal
deformation from the screw and products at locations immediately adjacent ponents, and most ratings were “trace” or
to the stainless steel “moderate.”
screw heads. This corroAt
the inspected curtain wall openings,
foam tapes
were found exclusively
along
spandrel sills
at the interface
between pressure
plates
and horizontal
mullions. In
general, there
was no correlation
between
the presence of
foam tape and
level of corrosion
activity in
the screw
Figure 8 – Condition of a site with severe corrosion:
A) before cleaning(above); B) after cleaning (right).
A
B
2 6 • C U I A N D S C H M I D T S Y M P O S I U M O N B U I L D I N G E N V E L O P E T E C H N O L O G Y • NO V E M B E R 2 0 0 7
chase. Powdery materials and foam tapes
were sampled for laboratory characterization.
Widespread water infiltration and water
retention within the horizontal mullions of
the curtain wall system were observed.
Pressure plate gasket shrinkage resulted in
gaps (see Figure 10A) for water penetration
into the glazing pockets. At three inspection
openings, water poured out of the glazing
pockets during removal of the horizontal
pressure plates. Figure 10B shows one of
ONSITE
TESTING
Chloride Test
Commercial chloride
testing kits were utilized
at selected horizontal
pressure plate surfaces
to determine whether or
not chloride was present.
As shown in Table 2,
Figure 9 – Varying corrosion
condition at pressure plate surface
around stainless steel screw: A) trace,
B) moderate, C) heavy, D) severe.
A
B
C
D
these openings with a significant quantity of chloride was consistently Screw PullOut
Testing
free water in the upper and lower glazing detected at sites with visible corrosion prodIn
an effort to quantify the probable
pockets, as well as in the screw chase. ucts and was not detected at sites that were screw connection strength loss associated
largely free of such products. with the localized aluminum corrosion of
A
B
Figure 10 – Evidence of water infiltration: A) avenue
for water penetration at shrinkage gap in gasket
(above); B) free water in glazing pockets and in
screw chase at an inspection opening (right).
S Y M P O S I U M O N B U I L D I N G E N V E L O P E T E C H N O L O G Y • NO V E M B E R 2 0 0 7 C U I A N D S C H M I D T • 2 7
Test
ID
Drop Floor Type of opening Surface with
powdery materials
(ppm)
Chloride
concentration
1 S2 8 3 No 0
2 E1 12 1 Yes 12
3 E1 10 3 Yes 27
4 E2 2 6 No 0
5 N1 13 2 Yes 47
6 N1 4 3 No 0
7 W2 1 6 Yes 30
8 W3 1 5 Yes 25
9 W4 14 4 No 0
Table 2 – Chloride test results performed on horizontal pressure plates.
1/64in
oversized chase (1/64in
oversize
in graph). This suggests that the screw
chase section loss induced by corrosion to
date is small (i.e., approximately equal to or
less than the effect of oversizing the screw
chase by 1/64 in).
LABORATORY TESTING OF POWDER
SAMPLES
SEM/EDS Test
A total of four corrosion product samples
(white powdery substances) were tested
using SEM/EDS. Two of the samples
were collected from the exterior surfaces of
two pressure plates, and the other two were
collected from the screw sites of two screw
chases. Regardless of sample location, each
sample was found to consist of some particles
that contained aluminum, oxygen, and
chlorine, and of some particles that contained
primarily aluminum and oxygen,
with only “trace” amounts or no chlorine. In
addition, some particles were found to be
primarily chloride salts, such as potassium
chloride. Figure 13 shows two examples of
the SEM micrographs and EDS spectra,
suggesting that the powders contain corrosion
products of aluminum mixed with
some chloride salts.
the screw chase, screw pullout
tests were
performed. After removal of the pressure
plate, selected screws were carefully threaded
into the serrated screw chase at the originally
installed locations and to the original
penetration depth. A custom apparatus,
shown in Figure 11A, was then attached to
the screw head. A slowly increasing tension
force was applied (see Figure 11B) until the
screw reached its maximum load. Tests
were performed on original screws at locations
with different corrosion ratings and on
new screws installed at new sites with no
corrosion.
Screw pullout
strength loss was generally
small. Table 3 shows the average values
for all the original screws and new screws.
The original screws had an average pullout
strength that was 1027 lbs, or 9 percent
less than the average value obtained for
new screws.
Figure 12 graphically presents the average
pullout
strength values for original
screws grouped according to the related
corrosion condition of associated screw
chase sites. Evidently, average screw pullout
strength decreases as the observed corrosion
condition worsens (from “trace” to
“severe”). The figure also shows the theoretical
strength values (calculated using the
procedure outlined in
AAMA TIRA91991
Metal Curtain Wall
Fasteners)1 for screws
installed in an optimumsized
screw chase (zero
oversize in graph) and
screws installed in a
Screw type Number of tests Average pullout
strength (lbs)
Original 40 1027
New 11 1134
A
B
Table 3 – Screw pullout
strengths.
Figure 11 – Screw pullout
test: A) the test apparatus;
B) a pullout
test in progress.
2 8 • C U I A N D S C H M I D T S Y M P O S I U M O N B U I L D I N G E N V E L O P E T E C H N O L O G Y • NO V E M B E R 2 0 0 7
Figure 12 – Average pullout
strength data for screws in horizontal mullion.
A
B
FTIR and XRD Tests
Two powder samples were also characterized
using the FTIR technique. However,
no conclusive information was derived from
this test. After completing SEM/EDS and
FTIR tests, XRD tests were performed on
the remaining powders of the two samples.
It was found that these powders were mostly
amorphous, and no peaks of crystalline
structure were positively identified.
Chloride Test
Six powder samples were weighed and
tested for chloride content using commercial
chloride testing kits. As shown in Table
4, the detected chloride content (0 to 2.4
percent) varies from sample to sample. This
is consistent with the EDS analyses (chloride
signal peak amplitude varied from particle
to particle).
The strong chlorine signal suggests that the
polymer is chlorinated.
Both tape samples appeared to be in
good condition with no sign of degradation.
They were flexible and would quickly return
to their original shape when compressed.
Figure 13 – Selected SEM micrographs
and EDS spectra: A) aluminum
corrosion products (Al and O) and
chlorine detected; B) chlorine and
potassium identified as primary
content (likely KCl salt).
Test ID Drop Floor Type of
opening
Sample mass
(g)
Chloride
concentration (wt %)
1 S2 1 5 0.0113 0
2 E2 8 3 0.0315 1.8
3 W2 9 3 0.0135 0
4 W2 1 6 0.0289 2.4
5 E1 10 3 0.0231 0.78
6 W4 3 3 0.0194 0.88
LABORATORY TESTING OF
FOAM TAPES
SEM/EDS Test
Two foam tape samples were
tested with SEM/EDS to identify
their compositions and to determine
whether or not the tapes are
sources of free chloride. As shown
in Figure 14, SEM/EDS analysis of
the foam tapes indicated signals
from carbon, chlorine, and calcium.
The calcium signal is likely
from the calcium carbonate filler. A
Table 4 – Chloride test results performed on corrosion product samples.
Figure 14 –
Selected SEM
micrographs and
point EDS spectra
of foam tape:
carbon, chlorine,
and calcium
detected in both A)
and B).
B
S Y M P O S I U M O N B U I L D I N G E N V E L O P E T E C H N O L O G Y • NO V E M B E R 2 0 0 7 C U I A N D S C H M I D T • 2 9
Figure 15 – Correlation between pullout
strength and corrosioninduced
section
loss. Measured pullout
strengths for horizontal mullions and 20year
projected
strength are also plotted.
FTIR Test
The FTIR results indicated the presence
of a phthalate plasticizer and calcium carbonate
filler. The sample was then extracted
with tetrahydrofuran (a solvent) in an
attempt to dissolve and analyze certain
chlorinated polymers. After extraction, only
the phthalate plasticizer (which was dissolved)
was detected. As the most likely
chlorinated polymer that is not soluble in
tetrahydrofuran is neoprene (polychloroprene),
it was speculated that the foam tape
material is likely a neoprene rubber with a
phthalate plasticizer.
While the analyses of the tapes suggest
that the polymer contained in the tapes is
chlorinated, the lack of degradation of the
foam tape, along with the inability to extract
chlorinated polymer, indicates that the tape
is not likely a source of free chloride.
Considering these findings and the fact that
there was no observed correlation between
the presence of the tape and corrosion
activity, it is unlikely that the tape is contributing
to the corrosion of the aluminum.
DISCUSSION
environment. A corrosion process typically
requires water and oxygen. It is widely
known that the presence of crevices,2
aggressive ions such as chloride,3 and a
more noble metal can result in severe localized
corrosion of a metal4 that would otherwise
remain passive. Unfortunately, the
horizontal aluminum mullions in this curtain
wall system have the following documented
characteristics that promote corrosion:
1. Widespread water infiltration and
water retention
2. Crevices at the interface between
screws and serrated screw chases
3. Presence of a more noble stainless
steel screw material (as compared to
the base aluminum)
4. Presence of free chloride (detected in
the corrosion products)
These factors (possibly also a synergistic
effect) are responsible for the observed
corrosion. The laboratory analyses suggest
that the detected free chloride did not originate
from the foam tape. Instead, the detection
of potassium chloride in the corrosion
product suggests that airborne deicing particles
are the most probable source of the
chloride.
CORROSIONINDUCED
SECTION LOSS
One of the consequences of corrosion is
the section loss of metal components. In the
case of screw chases, the impact of section
loss on pullout
strength can be reasonably
approximated by calculating the effects of
oversized screw chase. Figure 15 shows the
theoretical strength values (red solid circles)
corresponding to zero, 1/64in,
and 1/32in
oversize. These values were calculated
following the AAMA TIRA91991
procedure.
1 Assuming linearity between two adjacent
points, section loss induced by corrosion
can be estimated based on measured
pullout
strength values. Table 5 lists the
estimated section loss values corresponding
to each corrosion condition.
SERVICELIFE
PROJECTION
The impetus for this investigation was
concern regarding the longterm
effect of
the corrosion on the structural integrity of
the screwed pressure plate connections. A
lowerbound
(i.e., conservative) estimate of
the pullout
strength of the screws after
another 20 years of service can be predicted
by using the most severe current corrosion
condition and by assuming corrosion conPullout
strength (lbs) Estimated section loss (in)
New site pristine 1134 0.0037
Trace 1097 0.0047
Moderate 1037 0.0064
Heavy 996 0.0075
Severe 824 0.0123
Projection1 580 0.0210
CAUSES OF CORROSION
1 Assume severe corrosion condition.
Corrosion is the deterioration of a metal
due to its reaction with the surrounding
Table 5 – Estimated section loss and projected pullout
strength after 20 years of
additional service.
3 0 • C U I A N D S C H M I D T S Y M P O S I U M O N B U I L D I N G E N V E L O P E T E C H N O L O G Y • NO V E M B E R 2 0 0 7
tinuing over the next 20 years at a constant
rate equal to the corrosion rate that has
occurred over the past 20 years. (This
methodology is conservative because very
few of the screws presently have a severe
corrosion rating and because the scheduled
exterior sealant repairs will reduce water
infiltration, a response that should decrease
the corrosion rate in the future.) With this
methodology, after another 20 years of service,
the projected section loss was estimated
to be about 0.021 in and the projected
screw pullout
strength would be approximately
560 lb (Table 5). Figure 15 shows the
estimated section loss for screw sites with
various corrosion conditions and the projected
section loss after another 20 years of
service.
Under design wind loads (calculated per
the current governing ASCE 795
standard5),
the maximum load per fastener is
about 150 lb. Maximum screw loads occur
only at select locations, such as near building
corners and near the center of each
pressure plate. Average wind load per fastener
is somewhat less.
Table 6 shows the projected screw pullout
strength (calculated conservatively as
described above), the required maximum
strength to resist wind loads, and the
resulting projected factor of safety. As
shown, the calculations indicate that the
pressure plate screw connections will have
sufficient strength to resist current code
wind loads with an adequate factor of safety
(nearly 4.0) for at least the next 20 years.
It should be noted that future strength
loss of the screws that currently exhibit
“trace” to “moderate” corrosion can be estimated
with confidence based on the results
of this testing. However, future strength
loss of the screws that currently exhibit
severe corrosion is more difficult to predict
(i.e., additional strength loss for these
severe corrosion conditions may not be linear).
However, since severe corrosion conditions
only account for approximately 2 percent
of those inspected, the abovedescribed
methodology should be conservative.
Furthermore, even if the currentlyrated
severe corrosion screw sites provided no
windload
resistance in 20 years (i.e., if
these screws were to fail completely), the
remaining screw connections at their projected
strengths would still be capable of
resisting currentcode
wind loads with an
adequate factor of safety.
CONCLUSIONS
Based on the findings of the onsite
investigation and the laboratory testing, the
following conclusions can be drawn regarding
corrosion conditions at the screw connections
of the aluminum pressure plates
in the subject curtain wall system:
• Observed corrosion activity at the
screws along the millfinished
horizontal
mullions varied from “trace”
to “severe,” with the average condition
being in the trace to moderate
range. Slight to no corrosion activity
was observed along vertical mullions,
which were all painted.
• Foam tapes containing chlorinated
polymers were detected at spandrel
sill locations. The tapes are not likely
contributors to the aluminum corrosion.
• The conditions within glazing pockets
– including the presence of
water, detected free chloride, inherent
crevices, and dissimilar metals –
are favorable to corrosion.
• The source of the chlorides was not
determined in this study, but it is
suspected to be airborne particles of
deicing materials used on nearby
parking lots and roadways.
• Corrosion ratings correlate well with
screw pullout
strength loss.
• Based on conservative assumptions,
calculations indicate that the screw
connections will retain sufficient
strength to resist current coderequired
wind loads for at least
another 20 years.
• The observed corrosion conditions
and the corresponding screw pullout
strength losses did not warrant
imminent repair.
REFERENCES:
1. AAMA TIRA91991,
“Metal Curtain
Wall Fasteners,” American Architectural
Manufacturers Association,
Schaumburg, Illinois, 1991, pp. 1617
and 2000 Addendum.
2. R.G. Kelly, Crevice Corrosion, in: M.
Stratmann, G.S. Grankel (Eds.),
Encyclopedia of Electrochemistry
2003, vol. 4, WileyVCH
Verlag
GambH & Co. KGaA, Weinheim,
Germany, 2003, pp. 275.
3. F. Cui, F.J. PresuelMoreno,
R.G.
Kelly, “Experimental and Computational
Evaluation of the Protection
Provided by an Aluminum Cladding
to AA2024T3
Exposed at a Seacoast
Environment,” Corrosion 62 (3),
2006, pp. 252631.
4. L.J. Korb and D.L. Olson (Eds.),
Corrosion in Metals Handbook, vol.
13, ASM International, Metals Park,
Ohio, 1987, p. 83.
5. ASCE 795
Minimum Design Loads
for Buildings and Other Structures,
American Society of Civil Engineers,
Reston, Virginia, 1995, pp. 1234.
Table 6 – Projected and maximum required strengths.
Estimated/projected screw strengths Horizontal mullions1
and factors of safety
Pullout
strength – Current (lbs) 824
Projected pullout
strength – In 20 years (lbs) 580
Required maximum strength (lbs) 150
Conservative projected factor of safety in 20 years 3.8
1 Severe corrosion condition assumed.
S Y M P O S I U M O N B U I L D I N G E N V E L O P E T E C H N O L O G Y • NO V E M B E R 2 0 0 7 C U I A N D S C H M I D T • 3 1